You would be better off using canola oil, it's not as toxic and gives a faster quench. You want the oil at about 100 degrees if you live in a cold climate or your steel can crack(ask me how I know). If you haven't done any forging or welding on the 'points' you only need to heat it up to a non critical temp (a magnet won't be attracted to it at that temp) one time, and then get it into the oil as fast as you can. Once you've done that, clean em off and put in a preheated (450 degrees) oven for 30min and then into the oil again as fast as you can get it there. This should give you a chisel hard point, provided the steel is heat treatable. Not all steel will harden. If it won't harden than you can contact me and somewhere I have a formula for a solution that will case harden mild steel.......good luck.
Paul